鋁水澆包(bao)烘干工藝包(bao)括(kuo)如下步驟:
a)在(zai)鋁水(shui)澆(jiao)包(bao)外(wai)殼上(shang)均勻開設若干個(ge)直(zhi)徑為(wei)8-10mm的排氣(qi)孔,相鄰兩個(ge)排氣(qi)孔的圓心間距為(wei)200mm,在(zai)鋁水(shui)澆(jiao)包(bao)烘烤前進行檢查,保證(zheng)每個(ge)排氣(qi)孔暢(chang)通;
b)采(cai)用(yong)焦(jiao)(jiao)炭(tan)作(zuo)為燃(ran)(ran)料,焦(jiao)(jiao)炭(tan)放在燃(ran)(ran)燒(shao)裝(zhuang)(zhuang)(zhuang)置(zhi)的(de)圓(yuan)柱形爐膛內,鋁液除氣機(ji)供應,燃(ran)(ran)燒(shao)裝(zhuang)(zhuang)(zhuang)置(zhi)配(pei)備離心式(shi)鼓(gu)風(feng)機(ji),離心式(shi)鼓(gu)風(feng)機(ji)的(de)風(feng)量控制(zhi)在2-5m3/h;焦(jiao)(jiao)炭(tan)燃(ran)(ran)燒(shao)后,啟動離心式(shi)鼓(gu)風(feng)機(ji),從燃(ran)(ran)燒(shao)裝(zhuang)(zhuang)(zhuang)置(zhi)的(de)噴嘴內吹出火束,將鋁水(shui)澆包烘干(gan);
c)火束的(de)長度控(kong)制在600-800mm,鋁液(ye)除氣機價格,火束末端離(li)(li)開鐵(tie)水包底部(bu)的(de)距離(li)(li)為150-250mm;
冶煉行業鋁水(shui)澆(jiao)包(bao)(bao)是爐(lu)前(qian)出(chu)鋁的(de)主要(yao)設(she)備(bei),其使用(yong)壽命與包(bao)(bao)襯材質的(de)選擇和砌筑工藝有著直接關系。為了延(yan)長使用(yong)時間(jian),做到不(bu)漏(lou)包(bao)(bao),在鋁水(shui)澆(jiao)包(bao)(bao)上應用(yong)了耐火澆(jiao)注(zhu)料(liao),澆(jiao)注(zhu)鋁水(shui)澆(jiao)包(bao)(bao)內(nei)襯的(de)試(shi)驗,廣東鋁液除氣機(ji),分析了使用(yong)后的(de)利弊(bi)和注(zhu)意(yi)事(shi)項。
1、原耐火磚包襯結構及(ji)存在的問題
原(yuan)鋁水澆包(bao)由鋼殼和(he)內(nei)襯(chen)兩部分組成,殼體用鋼板制作,內(nei)襯(chen)用耐火材料(liao)砌筑。包(bao)襯(chen)一般使(shi)用包(bao)齡較短(duan),使(shi)用壽命短(duan)的(de)原(yuan)因有2種情況:一是(shi)由于局部燒穿(chuan),發生漏包(bao)現象;二(er)是(shi)隨著出(chu)鋁次數的(de)增加,包(bao)底粘有大量的(de)鋁渣形成包(bao)砣(tuo),鋁液包(bao)容積變(bian)小,再(zai)出(chu)鋁時鋁液坐包(bao),導致(zhi)包(bao)報廢。
2、鋁水澆包(bao)包(bao)襯澆注料的試(shi)制
耐火澆(jiao)(jiao)(jiao)(jiao)注(zhu)料在冶煉行(xing)(xing)業(ye)(ye),鍛造行(xing)(xing)業(ye)(ye)已應用十分廣泛。在鋁(lv)水澆(jiao)(jiao)(jiao)(jiao)包(bao)包(bao)襯澆(jiao)(jiao)(jiao)(jiao)注(zhu)料整體澆(jiao)(jiao)(jiao)(jiao)注(zhu)在冶煉行(xing)(xing)業(ye)(ye)一(yi)直(zhi)是個選(xuan)擇的難題。之前一(yi)直(zhi)是以耐火磚砌(qi)筑為主,為此(ci)需要(yao)研制(zhi)一(yi)種(zhong)能滿足冶煉行(xing)(xing)業(ye)(ye)鋁(lv)水澆(jiao)(jiao)(jiao)(jiao)包(bao)包(bao)襯的耐火澆(jiao)(jiao)(jiao)(jiao)注(zhu)料。
鋁(lv)水澆包(bao)的烘干
1.鋁水澆包大修后必須(xu)先陰干一(yi)段時(shi)間,避(bi)免因直接烘干造成修包材(cai)料產生嚴重(zhong)裂紋。
2.采用(yong)天然qi進(jin)行(xing)烘(hong)(hong)干(gan):≥10T包(bao)(bao)(bao)的(de)(de)烘(hong)(hong)干(gan)時(shi)(shi)(shi)間(jian)>10h;≥5T包(bao)(bao)(bao)的(de)(de)烘(hong)(hong)干(gan)時(shi)(shi)(shi)間(jian)>5h;≤5T包(bao)(bao)(bao)的(de)(de)烘(hong)(hong)干(gan)時(shi)(shi)(shi)間(jian)>3h;采用(yong)煤烘(hong)(hong)烤(kao)可在(zai)天然qi烘(hong)(hong)烤(kao)的(de)(de)時(shi)(shi)(shi)間(jian)基礎(chu)上,分別增(zeng)加2-4h;以保證鋁水澆包(bao)(bao)(bao)的(de)(de)充分干(gan)燥;在(zai)鋁水澆包(bao)(bao)(bao)使(shi)用(yong)前,還要進(jin)行(xing)“燙包(bao)(bao)(bao)”處(chu)理(li),用(yong)1450℃左右的(de)(de)鋁水將(jiang)剛(gang)進(jin)行(xing)了大修(xiu)的(de)(de)澆包(bao)(bao)(bao)裝滿,燙2-3次,使(shi)之充分干(gan)燥。